| AISI 410 | ||||
| Chemical composition: C=0.15%max, Mn=1%max, Cr=12.5% | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 7.7 *10³ | kg/m³ | 481 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 200 | GPa | 29000 | ksi |
| Thermal expansion (20 ºC) | 9.9*10-6 | ºCˉ¹ | 5.5*10-6 | in/(in* ºF) |
| Specific heat capacity | 460 | J/(kg*K) | 0.11 | BTU/(lb*ºF) |
| Thermal conductivity | 24.9 | W/(m*K) | 173 | BTU*in/(hr*ft²*ºF) |
| Electric resistivity | 5.7*10-7 | Ohm*m | 5.7*10-5 | Ohm*cm |
| Tensile strength (annealed) | 520 | MPa | 75400 | psi |
| Yield strength (annealed) | 275 | MPa | 40000 | psi |
| Elongation (annealed) | 30 | % | 30 | % |
| Hardness (annealed) | 82 | RB | 82 | RB |
| Tensile strength (cold drawn) | 834 | MPa | 121000 | psi |
| Yield strength (cold drawn) | 721 | MPa | 105000 | psi |
| Elongation (cold drawn) | 21 | % | 21 | % |
| Hardness (cold drawn) | 24 | RC | 24 | RC |