| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RD 100 Brale | R15N Brale | R30N Brale | R45N Brale | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Shore |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 92 | - | 80 | 87 | 97 | 92 | 87 | - | - | - | - | - | 1865 | - |
| 92 | - | 79 | 86 | 96 | 92 | 87 | - | - | - | - | - | 1787 | - |
| 91 | - | 78 | 85 | 96 | 91 | 86 | - | - | - | - | - | 1710 | - |
| 91 | - | 77 | 84 | 96 | 91 | 85 | - | - | - | - | - | 1633 | - |
| 90 | - | 76 | 83 | 96 | 90 | 84 | - | - | - | - | - | 1556 | - |
| 90 | - | 75 | 83 | 95 | 89 | 83 | - | - | - | - | - | 1478 | - |
| 89 | - | 74 | 82 | 95 | 89 | 82 | - | - | - | - | - | 1400 | - |
| 89 | - | 73 | 81 | 95 | 88 | 81 | - | - | - | - | - | 1323 | - |
| 88 | - | 72 | 80 | 95 | 87 | 80 | - | - | - | - | - | 1245 | - |
| 87 | - | 71 | 80 | 94 | 87 | 79 | - | - | - | - | - | 1160 | - |
| 87 | - | 70 | 79 | 94 | 86 | 78 | - | - | - | - | - | 1076 | 101 |
| 86 | - | 69 | 78 | 94 | 85 | 77 | - | - | - | - | - | 1004 | 99 |
| 85.6 | - | 68 | 76.9 | 93.2 | 84.4 | 75.4 | - | - | - | - | - | 940 | 97 |
| 85 | - | 67 | 76.1 | 92.9 | 83.6 | 74.2 | - | - | - | - | - | 900 | 95 |
| 84.5 | - | 66 | 75.4 | 92.5 | 82.8 | 73.3 | - | - | - | - | - | 865 | 92 |
| 83.9 | - | 65 | 74.5 | 92.2 | 81.9 | 72 | - | - | - | - | 739 | 832 | 91 |
| 83.4 | - | 64 | 73.8 | 91.8 | 81.1 | 71 | - | - | - | - | 722 | 800 | 88 |
| 82.8 | - | 63 | 73 | 91.4 | 80.1 | 69.9 | - | - | - | - | 705 | 772 | 87 |
| 82.3 | - | 62 | 72.2 | 91.1 | 79.3 | 68.8 | - | - | - | - | 688 | 746 | 85 |
| 81.8 | - | 61 | 71.5 | 90.7 | 78.4 | 67.7 | - | - | - | - | 670 | 720 | 83 |
| 81.2 | - | 60 | 70.7 | 90.2 | 77.5 | 66.6 | - | - | - | - | 613 | 697 | 81 |
| 80.7 | - | 59 | 69.9 | 89.8 | 76.6 | 65.5 | - | - | - | - | 599 | 674 | 80 |
| 80.1 | - | 58 | 69.2 | 89.3 | 75.7 | 64.3 | - | - | - | - | 587 | 653 | 78 |
| 79.6 | - | 57 | 68.5 | 88.9 | 74.8 | 63.2 | - | - | - | - | 575 | 633 | 76 |
| 79 | - | 56 | 67.7 | 88.3 | 73.9 | 62 | - | - | - | - | 561 | 613 | 75 |
| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RD 100 Brale | R15N Brale | R30N Brale | R45N Brale | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Shore |
| 78.5 | 120 | 55 | 66.9 | 87.9 | 73 | 60.9 | - | - | - | - | 546 | 585 | 74 |
| 78 | 120 | 54 | 66.1 | 87.4 | 72 | 59.8 | - | - | - | - | 534 | 577 | 72 |
| 77.4 | 119 | 53 | 65.4 | 86.9 | 71.2 | 58.6 | - | - | - | - | 519 | 560 | 71 |
| 76.8 | 119 | 52 | 64.6 | 86.4 | 70.2 | 57.4 | - | - | - | - | 500 | 544 | 69 |
| 76.3 | 118 | 51 | 63.8 | 85.9 | 69.4 | 56.1 | - | - | - | - | 487 | 528 | 68 |
| 75.9 | 117 | 50 | 63.1 | 85.5 | 68.5 | 55 | - | - | - | - | 475 | 513 | 67 |
| 75.2 | 117 | 49 | 62.1 | 85 | 67.6 | 53.8 | - | - | - | - | 464 | 498 | 66 |
| 74.7 | 116 | 48 | 61.4 | 84.5 | 66.7 | 52.5 | - | - | - | - | 451 | 484 | 64 |
| 74.1 | 116 | 47 | 60.8 | 83.9 | 65.8 | 51.4 | - | - | - | - | 442 | 471 | 63 |
| 73.6 | 115 | 46 | 60 | 83.5 | 64.8 | 50.3 | - | - | - | - | 432 | 458 | 62 |
| 73.1 | 115 | 45 | 59.2 | 83 | 64 | 49 | - | - | - | - | 421 | 446 | 60 |
| 72.5 | 114 | 44 | 58.5 | 82.5 | 63.1 | 47.8 | - | - | - | - | 409 | 434 | 58 |
| 72 | 113 | 43 | 57.7 | 82 | 62.2 | 46.7 | - | - | - | - | 400 | 423 | 57 |
| 71.5 | 113 | 42 | 56.9 | 81.5 | 61.3 | 45.5 | - | - | - | - | 390 | 412 | 56 |
| 70.9 | 112 | 41 | 56.2 | 80.9 | 60.4 | 44.3 | - | - | - | - | 381 | 402 | 55 |
| 70.4 | 112 | 40 | 55.4 | 80.4 | 59.5 | 43.1 | - | - | - | - | 371 | 392 | 54 |
| 69.9 | 111 | 39 | 54.6 | 79.9 | 58.6 | 41.9 | - | - | - | - | 362 | 382 | 52 |
| 69.4 | 110 | 38 | 53.8 | 79.4 | 57.7 | 40.8 | - | - | - | - | 353 | 372 | 51 |
| 68.9 | 110 | 37 | 53.1 | 78.8 | 56.8 | 39.6 | - | - | - | - | 344 | 363 | 50 |
| 68.4 | 109 | 36 | 52.3 | 78.3 | 55.9 | 38.4 | - | - | - | - | 336 | 354 | 49 |
| 67.9 | 109 | 35 | 51.5 | 77.7 | 55 | 37.2 | - | - | - | - | 327 | 345 | 48 |
| 67.4 | 108 | 34 | 50.8 | 77.2 | 54.2 | 36.1 | - | - | - | - | 319 | 336 | 47 |
| 66.8 | 108 | 33 | 50 | 76.6 | 53.3 | 34.9 | - | - | - | - | 311 | 327 | 46 |
| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RD 100 Brale | R15N Brale | R30N Brale | R45N Brale | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Shore |
| 66.3 | 107 | 32 | 49.2 | 76.1 | 52.1 | 33.7 | - | - | - | - | 301 | 318 | 44 |
| 65.8 | 106 | 31 | 48.4 | 75.6 | 51.3 | 32.5 | - | - | - | - | 294 | 310 | 43 |
| 65.3 | 105 | 30 | 47.7 | 75 | 50.4 | 31.3 | - | - | - | - | 286 | 302 | 42 |
| 64.7 | 104 | 29 | 47 | 74.5 | 49.5 | 30.1 | - | - | - | - | 279 | 294 | 41 |
| 64.3 | 104 | 28 | 46.1 | 73.9 | 48.6 | 28.9 | - | - | - | - | 271 | 286 | 40.5 |
| 63.8 | 103 | 27 | 45.2 | 73.3 | 47.7 | 27.8 | - | - | - | - | 264 | 279 | 40 |
| 63.3 | 103 | 26 | 44.6 | 72.8 | 46.8 | 26.7 | - | - | - | - | 258 | 272 | 38 |
| 62.8 | 102 | 25 | 43.8 | 72.2 | 45.9 | 25.5 | - | - | - | - | 253 | 266 | 37.5 |
| 62.4 | 101 | 24 | 43.1 | 71.6 | 45 | 24.3 | - | - | - | - | 247 | 260 | 37 |
| 62 | 100.5 | 23 | 42.1 | 71 | 44 | 23.1 | - | - | - | - | 243 | 254 | 36 |
| 61.5 | 100 | 22 | 41.6 | 70.5 | 43.2 | 22 | 93 | 82 | 72 | 201 | 237 | 248 | 251 |
| 61 | 99 | 21 | 40.9 | 69.9 | 42.3 | 20.7 | 92.5 | 81.5 | 71 | 195 | 231 | 243 | 246 |
| 60.5 | 98.5 | 20 | 40.1 | 69.4 | 41.5 | 19.6 | 92.4 | 81.2 | 70.5 | 192 | 228 | 238 | 243 |
| 60 | 98 | 20 | - | - | - | - | 92.3 | 81 | 70 | 189 | 226 | 237 | 241 |
| 59.5 | 97 | 19 | - | - | - | - | 92 | 80.5 | 69 | 184 | 222 | 234 | 236 |
| 59 | 96 | 18 | - | - | - | - | 91.8 | 80 | 68 | 179 | 216 | 230 | 231 |
| 58 | 95 | 16 | - | - | - | - | 91.5 | 79 | 67 | 175 | 210 | 222 | 226 |
| 57.5 | 94 | 14 | - | - | - | - | 91.3 | 78.5 | 66 | 171 | 205 | 213 | 221 |
| 57 | 93 | 13 | - | - | - | - | 91 | 78 | 65.5 | 167 | 200 | 208 | 216 |
| 56.5 | 92 | 11 | - | - | - | - | 90.5 | 77.5 | 64.5 | 163 | 195 | 200 | 211 |
| 56 | 91 | 10 | - | - | - | - | 90.8 | 77 | 63.5 | 160 | 190 | 196 | 206 |
| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RD 100 Brale | R15N Brale | R30N Brale | R45N Brale | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Shore |
http://www.virginia.edu/bohr/mse209/chapter6.htm
http://www.eng.auburn.edu/~wfgale/intro_metals/toc.htm
http://www.nde-ed.org/EducationResources/CommunityCollege/
Materials/Introduction/introduction.htm
http://www.ame.arizona.edu/courses/ame324b/l04.pdf
http://people.clarkson.edu/~rasmu/ES-260/Chapter_07.ppt
http://me.queensu.ca/courses/mech412/Notes/Review2.ppt