SubsTech     
SubsTech     

to Carbon steels
to Properties of steels and cast irons

Carbon steel SAE 1030

(submitted by the website administration)

SAE 1030
Chemical composition: C=0.30%, Mn=0.75%, P=0.04% max, S=0.05% max
Property Value in metric unit Value in US unit
Density 7.872 *10³ kg/m³ 491.4 lb/ft³
Modulus of elasticity 200 GPa 29000 ksi
Thermal expansion (20 ºC) 11.7*10-6 ºCˉ¹ 6.5*10-6 in/(in* ºF)
Specific heat capacity 486 J/(kg*K) 0.116 BTU/(lb*ºF)
Thermal conductivity 48.7 W/(m*K) 338 BTU*in/(hr*ft²*ºF)
Electric resistivity 1.66*10-7 Ohm*m 1.66*10-5 Ohm*cm
Tensile strength (hot rolled) 470 MPa 68200 psi
Yield strength (hot rolled) 260 MPa 37700 psi
Elongation (hot rolled) 20 % 20 %
Hardness (hot rolled) 75 RB 75 RB
Tensile strength (cold drawn) 525 MPa 76100 psi
Yield strength (cold drawn) 440 MPa 63800 psi
Elongation (cold drawn) 12 % 12 %
Hardness (cold drawn) 80 RB 80 RB

Related internal links

Related external links

carbon_steel_sae_1030.txt · Last modified: 2012/06/02 by dmitri_kopeliovich
Promote in SubsTech       Creative Commons License Except where otherwise noted, this work is licensed under a Creative Commons Attribution-Noncommercial-Share Alike 3.0 License