Carbon steel SAE 1010

(submitted by the website administration)

SAE 1010
Chemical composition: C=0.10%, Mn=0.45%, P=0.04% max, S=0.05% max
Property Value in metric unit Value in US unit
Density 7.872 *10³ kg/m³ 491.4 lb/ft³
Modulus of elasticity 200 GPa 29000 ksi
Thermal expansion (20 ºC) 12.6*10-6 ºCˉ¹ 7.00*10-6 in/(in* ºF)
Specific heat capacity 448 J/(kg*K) 0.107 BTU/(lb*ºF)
Thermal conductivity 51.9 W/(m*K) 360 BTU*in/(hr*ft²*ºF)
Electric resistivity 1.43*10-7 Ohm*m 1.43*10-5 Ohm*cm
Tensile strength (hot rolled) 325 MPa 47100 psi
Yield strength (hot rolled) 180 MPa 26100 psi
Elongation (hot rolled) 28 % 28 %
Hardness (hot rolled) 55 RB 55 RB
Tensile strength (cold drawn) 365 MPa 52900 psi
Yield strength (cold drawn) 305 MPa 44200 psi
Elongation (cold drawn) 20 % 20 %
Hardness (cold drawn) 60 RB 60 RB

Related internal links

Related external links

carbon_steel_sae_1010.txt · Last modified: 2012/06/02 by dmitri_kopeliovich
Promote in SubsTech       Creative Commons License Except where otherwise noted, this work is licensed under a Creative Commons Attribution-Noncommercial-Share Alike 3.0 License