Chemical composition: Sn=6.0%, Pb=1.5%, Zn=4.5%, Cu=88%
Property Value in metric unit Value in US unit
Density 8.64 *10³ kg/m³ 539 lb/ft³
Modulus of elasticity 96.5 GPa 14000 ksi
Thermal expansion (20 ºC) 18.0*10-6 ºCˉ¹ 10.0*10-6 in/(in* ºF)
Specific heat capacity 377 J/(kg*K) 0.090 BTU/(lb*ºF)
Thermal conductivity 69.6 W/(m*K) 482 BTU*in/(hr*ft²*ºF)
Electric resistivity 12.0*10-8 Ohm*m 12.0*10-6 Ohm*cm
Tensile strength (sand cast) 276 MPa 40000 psi
Yield strength (sand cast) 138 MPa 20000 psi
Elongation (sand cast) 30 % 30 %
Fatigue strength (sand cast) 76 MPa 11000 psi
Hardness (sand cast) 65 HB(500) 65 HB(500)
Liquidus temperature 988 ºC 1810 ºF
Solidus temperature 826 ºC 1518 ºF