| Elastomer | ||||
| Hypalon (CSM, Chlor-Sulfonated Polyethylene) | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 1.2 *10³ | kg/m³ | 74.9 | lb/ft³ | 
|---|---|---|---|---|
| Tensile strength | 21 | MPa | 3050 | psi | 
| Elongation | 500 | % | 500 | % | 
| Glass transition temperature | -55 | ºC | -67 | ºF | 
| Maximum work temperature | 130 | ºC | 266 | ºF | 
| Electric resistivity | 106 | Ohm*m | 108 | Ohm*cm | 
| Dielectric constant | 8.5 | - | 8.5 | - | 
Applications: cable insulation, gaskets, flexible hoses for oil and chemicals, conveyor belts.