Wrought aluminum alloy 1350
Chemical composition: Si=0.1%, Fe =0.40% , Al=99.5% min
Property Value in metric unit Value in US unit
Density 2.705 *10³ kg/m³ 169 lb/ft³
Modulus of elasticity 69 GPa 10000 ksi
Thermal expansion (20 ºC) 23.8*10-6 ºCˉ¹ 13.2*10-6 in/(in* ºF)
Specific heat capacity 900 J/(kg*K) 0.215 BTU/(lb*ºF)
Thermal conductivity 234 W/(m*K) 1625 BTU*in/(hr*ft²*ºF)
Electric resistivity 2.83*10-8 Ohm*m 2.83*10-6 Ohm*cm
Tensile strength (annealed) 83 MPa 12000 psi
Yield strength (annealed) 28 MPa 4000 psi
Elongation (annealed) 23 % 23 %
Shear strength (annealed) 55 MPa 8000 psi
Hardness (annealed) 23 HB 23 HB
Tensile strength (H16) 124 MPa 18000 psi
Yield strength (H16) 110 MPa 16000 psi
Elongation (H16) 3 % 3 %
Shear strength (H16) 76 MPa 11000 psi
Hardness (H16) 34 HB 34 HB
Annealing temperature 343 ºC 650 ºF