Alkyds (AMC), mineral filled
Property Value in metric unit Value in US unit
Modulus of elasticity 12 GPa 1800 ksi
Tensile strength 45 MPa 6500 psi
Flexural yield strength 90 MPa 13000 psi
Compressive strength 170 MPa 25000 psi
Thermal expansion (20 ºC) 36*10-6 ºCˉ¹ 20*10-6 in/(in* ºF)
Maximum work temperature 190 ºC 375 ºF

Applications: circuit breakers, switch gears, colored parts.