Composition: Silicon carbon (SiC) matrix + SiC long (cont.) fibers (14 mkm diameter)
Property Value in metric unit Value in US unit
Density 2.55 *10³ kg/m³ 159 lb/ft³
Modulus of elasticity 195 GPa 28300 ksi
Tensile strength 220 MPa 31900 psi
Thermal expansion (20 ºC) 3.2*10-6 ºCˉ¹ 1.8*10-6 in/(in* ºF)
Thermal heat capacity 630 J/(kg*K) 0.15 BTU/(lb*ºF)
Thermal conductivity 1.5 W/(m*K) 10.4 BTU*in/(hr*ft²*ºF)