Commercially pure nickel 301
Chemical composition: Al=4.4%, Ti=0.6%, Ni balance
Property Value in metric unit Value in US unit
Density 8.26 *10³ kg/m³ 516 lb/ft³
Modulus of elasticity 207 GPa 30000 ksi
Thermal expansion (20 ºC) 12.9*10-6 ºCˉ¹ 7.2*10-6 in/(in* ºF)
Specific heat capacity 435 J/(kg*K) 0.104 BTU/(lb*ºF)
Thermal conductivity 40.4 W/(m*K) 280 BTU*in/(hr*ft²*ºF)
Electric resistivity 42.4*10-8 Ohm*m 42.4*10-6 Ohm*cm
Tensile strength (annealed) 462 MPa 67000 psi
Yield strength (annealed) 148 MPa 21500 psi
Elongation (annealed) 45 % 45 %
Solution temperature 925 ºC 1700 ºF
Aging temperature 588 ºC 1090 ºF
Aging time 16 Hrs. 16 Hrs.