to Cast silicon bronzes and silicon brasses
to Properties of copper alloys

Cast copper alloy C87600 (Silicon Bronze/Silicon Brass)

(submitted by the website administration)

Cast copper alloy C87600 (Silicon Bronze/Silicon Brass)
Chemical composition: Zn=5.5%, Si=4.5%, Cu=90%
Property Value in metric unit Value in US unit
Density 8.30 *10³ kg/m³ 518 lb/ft³
Modulus of elasticity 117 GPa 17000 ksi
Specific heat capacity 377 J/(kg*K) 0.090 BTU/(lb*ºF)
Thermal conductivity 28.4 W/(m*K) 197 BTU*in/(hr*ft²*ºF)
Electric resistivity 23.0*10-8 Ohm*m 23.0*10-6 Ohm*cm
Tensile strength (sand cast) 455 MPa 66000 psi
Yield strength (sand cast) 221 MPa 32000 psi
Elongation (sand cast) 20 % 20 %
Hardness (sand cast) 135 HB(3000) 135 HB(3000)
Liquidus temperature 971 ºC 1780 ºF
Solidus temperature 860 ºC 1580 ºF

Related internal links


to Cast silicon bronzes and silicon brasses
to Properties of copper alloys