to Cast aluminum alloys
to Properties of aluminum alloys

Cast aluminum alloy 333.0

(submitted by the website administration)

Cast aluminum alloy 333.0
Chemical composition: Si=9.0%, Cu=3.5%, Mg=0.28%, Al balance, permanent mold casting
Property Value in metric unit Value in US unit
Density 2.77 *10³ kg/m³ 173 lb/ft³
Modulus of elasticity 73 GPa 10600 ksi
Thermal expansion (20 ºC) 20.5*10-6 ºCˉ¹ 11.4*10-6 in/(in* ºF)
Specific heat capacity 963 J/(kg*K) 0.230 BTU/(lb*ºF)
Thermal conductivity 105 W/(m*K) 725 BTU*in/(hr*ft²*ºF)
Electric resistivity 6.6*10-8 Ohm*m 6.6*10-6 Ohm*cm
Heat of fusion 3.89*105 J/kg 167 BTU/lb
Liquidus temperature 585 ºC 1085 ºF
Solidus temperature 516 ºC 960 ºF
Tensile strength (F), min. 193 MPa 28000 psi
Shear strength (F) 119 MPa 17300 psi
Hardness (F) , range 65-100 HB 65-100 HB
Tensile strength (T6), min 241 MPa 35000 psi
Shear strength (T6) 147 MPa 21300 psi
Hardness (T6) , range 85-115 HB 85-115 HB

Related internal links

Related external links

http://www.tntech.edu/me/courses/Zhang/ME30103110/Chap11pt4.ppt
http://www.ccm.udel.edu/Personnel/homepage/class_web/Lecture%20Notes/2004/AskelandPhuleNotes- CH13Printable.ppt
http://www.aluminum.org/
http://www.aluminium.org/
http://www.cmse.ed.ac.uk/MSE3/Topics/MSE3-nonferrous.pdf
http://www.ndt-ed.org/GeneralResources/MaterialProperties/ET/et_matlprop_index.htm

to Cast aluminum alloys
to Properties of aluminum alloys